Mässing
Icke-magnetisk legering av koppar och zink, men även andra legeringsämnen förekommer.
Densitet: 8,73 g/cm³ (max.)
Smältpunkt: 900-940°C
Legeringar
ALMAG S.P.A. - Mässing för maskinbearbetning och varmformning
Material | Cu | Pb | Sn | Fe | Ni | Al | Mn | As | Si | P | Zn | Other | Designation and Ref. Standard | Notes | |
36Pb3 | Min | 60 | 2,5 | - | - | - | - | - | - | - | - | Diff. | - | CW603N / CuZn36Pb3 | Standard alloy in the USA for machining with chip removal. Included in 4MS Positive List. |
Max | 62 | 3,5 | 0 | 0,3 | 0,2 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
37P | Min | 61 | - | - | - | - | - | - | - | - | 0,1 | Diff. | - | C27451 / CuZn37P | Dezincification resistant alloy with low lead content. Compliant to USA market. |
Max | 65 | 0,3 | - | 0,4 | - | - | - | - | - | 0,2 | - | 0,2 | _ | ||
39Pb3 | Min | 57 | 2,5 | - | - | - | - | - | - | - | - | Diff. | - | CW614N / CuZn39Pb3 | Standard alloy for machining with chip removal. It is included in 4MS Positive List. |
Max | 59 | 3,5 | 0 | 0,3 | 0,2 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
39Pb3-HS | Min | 57 | 2,5 | - | - | - | - | - | - | - | - | Diff. | - | CW614N / CuZn39Pb3 | Standard alloy for High Speed machining with chip removal. Recommended for round brass rods.Included in 4MS Positive List. |
Max | 59 | 3,5 | 0 | 0,3 | 0,2 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
60/40 Pb | Min | 59 | - | - | - | - | - | - | - | - | - | Diff. | - | CW509L / CuZn40 | High copper and reduced lead alloy. Included in 4MS Postive List. |
Max | 62 | 0,2 | 0 | 0,2 | 0,2 | 0,1 | - | - | - | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
607N | Min | 60 | 0,8 | - | - | - | - | - | - | - | - | Diff. | - | CW607N / CuZn38Pb1 | Medium-copper alloy with reduced lead. |
Max | 61 | 1,6 | 0 | 0,2 | 0,3 | 0,1 | - | - | - | - | - | 0,2 | DM 174 06/04/2004 | ||
610 | Min | 59 | 0,2 | - | - | - | - | - | - | - | - | Diff. | - | CW610N / CuZn39Pb0,5 | Leaded Muntz Metal. |
Max | 61 | 0,8 | 0 | 0,2 | 0,3 | 0,1 | - | - | - | - | - | 0,2 | DM 174 06/04/2004 | ||
708R | Min | 66 | - | - | - | - | - | - | - | 1 | - | Diff. | - | CW708R / CuZn31Si | Special alloy with high mechanical resistance and wear resistance. High-copper alloy. |
Max | 70 | 0,8 | - | 0,4 | 0,5 | - | - | - | 1 | - | - | 0,2 | - | ||
713R | Min | 57 | 0,2 | - | - | - | 1,3 | 1,5 | - | 0 | - | Diff. | - | CW713R / CuZn37Mn3AI2PbSi | Special alloy with high mechanical resistance and wear resistance. |
Max | 59 | 0,8 | 0 | 1 | 1 | 2,3 | 3 | - | 1 | - | - | 0,2 | - | ||
C363 | Min | 61 | 0,3 | - | - | - | - | - | - | - | 0 | Diff. | - | C36300 | Antidezincifying alloy with low lead content and without arsenic. |
Max | 63 | 0,7 | - | 0,2 | - | - | - | - | - | 0,2 | - | 0,2 | - | ||
C67300 | Min | 59 | 0,4 | - | - | - | - | 2 | - | 1 | - | Diff. | - | C67300 | Special anti-friction and wear-resistant alloy. |
Max | 63 | 3 | - | 0,5 | 0,3 | 0,3 | 3,5 | - | 2 | - | - | 0,2 | - | ||
CZ-LL | Min | 62 | - | - | - | - | - | - | 0 | - | - | Diff. | - | CW511L / CuZn38As | Anti-dezincification alloy for the USA market. Certified NSF372 and included in 4MS Positive List. |
Max | 64 | 0,2 | 0 | 0,1 | 0,3 | 0,1 | - | 0,2 | - | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
CZ-NL | Min | 62 | - | - | - | - | - | - | 0 | - | - | Diff. | - | CW511L / CuZn38As | Standard anti-dezincification alloy lead-free. It is included in 4MS Positive List. |
Max | 64 | 0,1 | 0 | 0,1 | 0,3 | 0,1 | - | 0,2 | - | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
CZ129 | Min | 59 | 0,8 | - | - | - | - | - | - | - | - | Diff. | - | CW611N / CuZn39Pb1 | Lead alloy for hot forging. |
Max | 60 | 1,6 | - | 0,3 | 0,3 | 0,1 | - | - | - | - | - | 0,2 | - | ||
CZ132 | Min | 61 | 1,7 | - | - | - | - | - | 0 | - | - | Diff. | - | CW602N / CuZn36Pb2As | Standard Anti-dezincification alloy. |
Max | 63 | 2,8 | 0 | 0,1 | 0,3 | 0,1 | 0,1 | 0,2 | - | - | - | 0,2 | DM 174 06/04/2004 | ||
CZA25 | Min | 62 | 1,2 | - | - | - | 0,5 | - | 0 | - | - | Diff. | - | CW625N / CuZn35Pb1,5AIAs | Standard anti-dezincification alloy. Included in 4MS Positive List. |
Max | 64 | 1,6 | 0 | 0,3 | 0,2 | 0,7 | 0,1 | 0,2 | - | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
CZA26 | Min | 64 | 1,2 | - | - | - | 0,8 | - | 0 | - | - | Diff. | - | CW626N / CuZn33Pb1,5AIAs | Standard anti-dezincification alloy. Included in 4MS Positive List. |
Max | 66 | 1,7 | 0 | 0,3 | 0,2 | 1 | 0,1 | 0,2 | - | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
EURO | Min | 57 | 1,6 | - | - | - | - | - | - | - | - | Diff. | - | CW617N / CuZn40Pb2 | Standard alloy with high workability. Included in 4MS Positive List. |
Max | 59 | 2,2 | 0 | 0,3 | 0,1 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
EURO-HS | Min | 57 | 1,6 | - | - | - | - | - | - | - | - | Diff. | - | CW617N / CuZn40Pb2 | High workability alloy and reduced lead content. It is included in the 4MS Positive List. |
Max | 59 | 2,2 | 0 | 0,3 | 0,1 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
FAB | Min | 57 | 2,2 | - | - | - | - | - | - | - | - | Diff. | - | CW617N / CuZn40Pb2 | Standard alloy for hot stamping with lead > 2,2%. |
Max | 59 | 2,5 | 0 | 0,3 | 0,3 | 0,1 | - | - | - | - | - | 0,2 | DM 174 06/04/2004 | ||
GSM | Min | 59 | 1,6 | - | - | - | - | - | - | - | - | Diff. | - | CW612N / CuZn39Pb2 | Standard high copper content alloy for free machining. Included in 4MS Positive List. |
Max | 60 | 2,2 | 0 | 0,3 | 0,1 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
LFB | Min | 57 | - | - | - | - | - | - | - | - | - | Diff. | - | CW510L / CuZn42 | Alloy with low lead content. Certified NSF372 for USA market. Included in 4MS Positive List. |
Max | 59 | 0,2 | 0 | 0,3 | 0,2 | 0,1 | - | - | - | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
MSPB2 | Min | 57 | 1,6 | - | - | - | - | - | - | - | - | Diff. | - | CW617N / CuZn40Pb2 | Standard alloy for hot forging with lead < 2%. Included in 4MS Positive List. |
Max | 59 | 2 | 0 | 0,3 | 0,1 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
NB (Navale - Naval) | Min | 59 | - | 1 | - | - | - | - | - | - | - | Diff. | - | CW719R / CuZn39Sn1 | Special alloy with high mechanical and corrosion resistance. Classic material for naval use. |
Max | 61 | 0,2 | 1 | 0,1 | 0,2 | - | - | - | - | - | - | 0,2 | _ | ||
NLB | Min | 57 | - | - | - | - | - | - | - | - | - | Diff. | - | CW510L / CuZn42 DIN 50930-6 | Lead-free alloy with optimized workability. |
Max | 59 | 0,1 | 0 | 0,3 | 0,2 | 0,1 | - | - | - | - | - | 0,2 | DM 174 06/04/2004 | ||
OT60/40 | Min | 59 | - | - | - | - | - | - | - | - | - | Diff. | - | CW509L / CuZn40 | High copper content and low lead content alloy, also known as Muntz metal. Compliant to USA market. Included in 4MS Positive List. |
Max | 62 | 0,1 | 0 | 0,2 | 0,2 | 0,1 | - | - | - | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
OT/63 | Min | 62 | - | - | - | - | - | - | - | - | - | Diff. | - | CW508L / CuZn37 | High cold deformability alloy. Included in 4MS Positive List. |
Max | 64 | 0,1 | 0 | 0,1 | 0,2 | 0,1 | - | - | - | - | - | 0,2 | - | ||
OTS D | Min | 57 | 0,2 | - | - | - | 0,3 | 0,8 | - | 0 | - | Diff. | - | CW718R / CuZn39Mn1AlPbSi | Special alloy with high mechanical resistance and wear resistance. |
Max | 59 | 0,8 | 1 | 0,5 | 0,5 | 1,3 | 1,8 | - | 1 | - | - | 0,2 | - | ||
PS | Min | 59 | 1,6 | - | - | - | - | - | - | - | - | Diff. | - | CW612N / CuZn39Pb2 | Standard high copper content alloy. Included in 4MS Positive List. |
Max | 60 | 2,2 | 0 | 0,3 | 0,1 | 0,1 | - | - | 0 | - | - | 0,2 | DIN 50930-6 / DM 174 06/04/2004 | ||
QQB | Min | 60 | 1,6 | - | - | - | - | - | - | - | - | Diff. | - | CW608N / CuZn38Pb2 | Standard high copper content alloy for chip removal. |
Max | 61 | 2,5 | 0 | 0,2 | 0,3 | 0,1 | - | - | - | - | - | 0,2 | DM 174 06/04/2004 | ||
SYD | Min | 64 | 0,4 | - | - | - | 0,1 | - | 0,1 | 0 | - | Diff. | - | CW725R / CuZn33Pb1AISiAs | Anti-dezincification alloy with low lead release. Included in the 4MS Positive List. |
Max | 67 | 0,6 | 0 | 0,3 | 0,2 | 0,4 | 0,1 | 0,1 | 0 | 0 | - | 0,2 | DM 174 06/04/2004 |